With Silver Nitrate added I call this glaze Silver Slither, which is pictured. This glaze has to be fired hot to about 1950F for the platelets to form beads. it looks different on top of a variety of base glazes as you can see from the photos. Works best on shoulder of pieces or on a more horizontal surface. Mix on the thick side. I usually apply a very small amount at a time by either pouring or brushing. When I pour it, I often will blow on it to move it around.
Raku Pottery Glaze Recipe
Frit 3110 85%
Nepheline Syenite 5
EPK 10
Add:
Tin Oxide 7
Magnesium Carbonate 34
Hectorite 2 or Bentonite 1
Optional: Silver Nitrate 2